SSD Notes: Fabrication of Semiconductor Devices

Nov 19, 2026·Pranesh Mahanta·21ECC201T — Solid State Devices

How an idea becomes a chip: integrated-circuit classes and their economics, crystal growth, wafer processing, oxidation, lithography, doping, and the planar fabrication of diodes, BJTs and MOSFETs.

Contents
  1. The integrated circuit: advantages and limitations
  2. Classification of integrated circuits
  3. Material preparation: from sand to electronic-grade silicon
  4. Crystal growing: the Czochralski process
  5. Wafer preparation
  6. Thermal oxidation and the Deal–Grove model
  7. Photolithography and pattern transfer
  8. Diffusion and ion implantation
  9. Fabrication of the PN junction diode
  10. Fabrication of the BJT
  11. Fabrication of the MOSFET
  12. Testing: wafer probing and yield
  13. Bonding and packaging

1The integrated circuit: advantages and limitations

An integrated circuit (IC) is a complete circuit — transistors, diodes, resistors and their interconnections — fabricated simultaneously within and on a single chip of semiconductor, rather than being assembled from discrete parts on a board. The planar process builds every device from the same small set of steps (oxidise, pattern, dope, deposit) repeated in sequence, so complexity costs almost nothing in area and the whole circuit is born as one monolithic piece of silicon.

Advantages: drastic size and weight reduction (millions of devices per square centimetre); low per-function cost because thousands of identical chips are processed in parallel; very high speed from micrometre-scale interconnects; low power; high reliability (no soldered joints, thermally matched materials, guarded parameters); and batch economy — hundreds of chips per wafer. Limitations: inductors and transformers cannot be integrated practically (only tiny values, poor Q); resistor and capacitor values are limited (kΩ, pF ranges) with poor tolerance (±10–20%) and positive temperature coefficients; high-power handling is excluded by heat density and breakdown; device parameters cannot be trimmed individually after fabrication; and design/layout cost is enormous, so ICs pay off only at volume.

The rule of thumb examiners like: ICs excel at repeating small, matched devices (transistors are cheap and nearly identical; resistors and capacitors are expensive and sloppy). Good monolithic design therefore uses transistors wherever possible and exploits the excellent matching (not absolute accuracy) of on-chip components.

2Classification of integrated circuits

ICs are classified two ways: by construction and by device count. By construction: monolithic ICs form all elements inside one silicon chip (the standard); thin-film/thick-film circuits deposit passive components as films on an insulating substrate with discrete devices attached (used for precision resistors and high power); hybrid ICs combine a monolithic chip (or chips) with film components and discrete parts in one package, covering the gap where monolithic technology cannot reach.

By complexity: SSI (small-scale, up to ≈10 gates: basic logic), MSI (medium, 10–100: counters, adders), LSI (large, 100–105: memories, early microprocessors), VLSI (very large, 105–109: CPUs, SoCs) and today ULSI with billions of transistors. A parallel split is by active-device type: bipolar (TTL, ECL — fast, power-hungry) versus MOS (CMOS — near-zero static power, dense, and the basis of virtually all modern logic).

ClassDevices per chipTypical examples
SSI< 100 transistors (≤ 12 gates)7400-series logic gates, flip-flops
MSI100–999Counters, shift registers, ALUs, decoders
LSI1k–10k4/8-bit microprocessors, early DRAMs, calculators
VLSI / ULSI10k–109+ Modern CPUs, GPUs, SoCs, gigabit memories

3Material preparation: from sand to electronic-grade silicon

Device-grade silicon begins as quartzite (SiO2). Carbothermic reduction in an electric arc furnace with coke and wood chips yields metallurgical-grade silicon (MG-Si) at about 98–99% purity — far too contaminated for devices, where dopants are measured in parts per billion. MG-Si is then ground and reacted with HCl to form trichlorosilane SiHCl3 (b.p. 31.8 °C), a liquid that can be fractionally distilled to extreme purity.

Chemical vapour deposition of the purified SiHCl3 on hot polysilicon seed rods at about 1100 °C (SiHCl3 + H2 → Si + 3HCl) produces electronic-grade silicon (EGS): 99.9999999% pure ("nine nines") polysilicon with electrical-grade impurity levels below 1 ppb. This polysilicon is the feedstock for single-crystal growth. The economics are striking: quartz to EGS multiplies the price a hundredfold, and EGS to finished device-grade crystal again many times — purity is the product.

SiO2 + 2C → Si + 2CO   (arc furnace, MG-Si ≈ 99%)
Si + 3HCl → SiHCl3 + H2   (purify by distillation)
SiHCl3 + H2 → Si + 3HCl   (CVD at ≈1100 °C, EGS > 99.9999999%)
Why silicon and not germanium for the industry: SiO2 forms a stable, patternable native oxide (essential to the planar process), Si keeps working to ≈200 °C (Ge gives up near 100 °C), and sand is cheaper than germanium ore by orders of magnitude.

4Crystal growing: the Czochralski process

Devices need single-crystal silicon — grain boundaries in polycrystalline material would swallow carriers and leak. The dominant growth technique is the Czochralski (CZ) process: EGS polysilicon is melted in a quartz crucible at about 1420 °C under an inert argon atmosphere, and a small single-crystal seed with the desired orientation (typically [100]) is dipped into the melt. The seed is rotated and slowly withdrawn while the melt solidifies onto it, copying its crystal orientation atom by atom. After an initial rapid pull forms a narrow neck (to dislocate-free the crystal), the pull rate is reduced so the crystal expands to full diameter (the crown), then grows as a cylindrical ingot (boule), tapering at the end (tail).

Pull rate 0.5–2 mm/min, rotation 10–40 rpm, growth along [100];   doping by adding weighed dopant to the melt (e.g. boron for p-type)
Diameter is controlled by pulling speed: pull faster → crystal narrows; pull slower → it widens. Modern auto-diameter control uses an infrared sensor watching the melt/crystal meniscus.

Doping is set by adding a weighed amount of dopant (phosphorus or boron) to the melt; because segregation keeps most impurities in the liquid, the ingot is slightly doped from the seed end to the tail — resistivity gradients of a few percent along the length are normal. The competing float-zone (FZ) process sweeps a molten zone through a polysilicon rod with no crucible contact, giving lower oxygen contamination and higher purity, but CZ wafers are cheaper, larger (300 mm and beyond) and good enough for the overwhelming majority of devices.

seed crystal single-crystal ingot silicon melt, ≈1420 °C quartz crucible heater argon atmosphere pull 0.5–2 mm/min rotate
Figure — Czochralski crystal puller: a rotating seed is dipped into the doped melt and withdrawn slowly, growing the single-crystal ingot (boule) that will be sliced into wafers.

5Wafer preparation

The CZ ingot is ground to exact diameter on an outer-diameter grinder, and flats or notches are ground along its length: they identify the crystallographic orientation and doping type, and give lithography its alignment reference. The ingot is then sliced into wafers on wire saws — hundreds of simultaneous cuts through a slurry of abrasive — along precisely oriented crystal planes ((100) or (111)). Slicing leaves wafers rough, tapered and damaged, so a refinement chain follows: lapping (alumina abrasive, flattens to a few micrometres), edge rounding (prevents chipping), chemical-mechanical polishing (alkaline slurry on a rotating pad) to a defect-free mirror finish, then final chemical cleaning (RCA cleans) to strip metals and organics.

Wafers per ingot ≈ L/(t + k),   t = wafer thickness, k = saw kerf loss
Typical polish wafer: 200–300 mm diameter, 500–800 µm thick; specification tolerances are in micrometres of flatness across the whole wafer — lithography depends on it.
Worked example · wafers per ingot
A Czochralski boule of 150 mm diameter yields 900 mm of usable single-crystal length. Wafers are sliced 600 µm thick and the wire-saw kerf wastes 25 µm per cut. How many wafers does the ingot yield, and what is the total wafer surface area processed?
Pitch per wafer: thickness + kerf = 600 + 25 = 625 µm = 0.625 mm.
Wafers: N = 900 mm/0.625 mm = 1440 wafers.
Surface area per wafer: πr² with r = 7.5 cm: π × 56.25 = 176.7 cm² per wafer.
Total area: 1440 × 176.7 cm² = 254,450 cm² ≈ 25.4 m² of silicon surface — every square centimetre of which must end up defect-free.
Check: the kerf wastes 25/625 = 4% of the ingot length; lapping and polishing remove another few micrometres per side before devices are ever started.

6Oxidation and the Deal–Grove model

Thermal oxidation grows SiO2 on silicon by exposing the wafer to O2 (dry) or H2O (wet) steam at 900–1200 °C in a furnace. The oxide is not deposited but consumes silicon: of the final thickness, 44% sits above the original surface and 56% below it — a detail that matters when aligning successive masks. The layer serves as mask against dopants, passivation against ionic contamination, dielectric for MOS gates, and insulation between interconnects.

Deal–Grove: x² + Ax = B(t + τ),   with A = B/(B/A)
Short time (interface-reaction limited): x ≈ (B/A)t  |  Long time (diffusion limited): x ≈ √(Bt)

The Deal–Grove model splits growth into three fluxes — gas transport to the surface, diffusion of the oxidant through the already-grown oxide, and reaction at the Si/SiO2 interface. Early on, the interface reaction limits growth (linear regime, rate constant B/A); as the oxide thickens, diffusing through it dominates (parabolic regime, rate constant B). Wet oxidation is 10–20× faster than dry but slightly porous — dry oxygen is reserved for critical gate oxides, wet steam for thick field and masking oxides. For sub-3 nm modern gates, thermal growth has given way to deposited high-k dielectrics (HfO2) to keep gate leakage in check.

Worked example · oxide growth time
A wet oxidation run at 1000 °C on bare silicon has rate constants B = 0.2 µm²/h and B/A = 0.5 µm/h (so A = 0.4 µm). Taking τ = 0, find the time needed to grow (a) a 0.4 µm masking oxide and (b) a 0.6 µm field oxide.
(a) x = 0.4 µm: x² + Ax = 0.16 + 0.4 × 0.4 = 0.16 + 0.16 = 0.32 µm².
t = 0.32/B = 0.32/0.2 = 1.6 h.
(b) x = 0.6 µm: x² + Ax = 0.36 + 0.4 × 0.6 = 0.36 + 0.24 = 0.60 µm².
t = 0.60/0.2 = 3.0 h.
Check: the pure-parabolic shortcut t = x²/B would give 0.16/0.2 = 0.8 h and 1.8 h — too short, because the linear term Ax is still significant at these thicknesses. Growth slows with thickness: doubling the target more than doubles the time (1.6 h → 3.0 h).

7Photolithography and pattern transfer

Photolithography transfers a drawn pattern onto the wafer and is repeated for every layer of the circuit. The sequence: spin-coat a light-sensitive photoresist (0.5–2 µm) over the wafer; soft-bake; expose through a photomask with UV light (contact/proximity printing, or a projection stepper that images one reticle field at a time, stepping across the wafer); develop — positive resist dissolves where exposed (negative resist, where unexposed); hard-bake to toughen the remaining resist. The patterned resist then protects the underlying film or oxide while the open areas are etched; finally the resist is stripped.

Resolution ≈ k1·λ/NA   (wavelength λ, numerical aperture NA of the projection optics)

Resolution improves with shorter wavelength — the industry went from 436 nm g-line and 365 nm i-line mercury lamps to 248 nm KrF and 193 nm ArF excimer lasers (now with water-immersion boosting NA > 1) — and with optics, chemistry (resolution-enhancement techniques) and EUV at 13.5 nm for leading-edge nodes. Mask alignment matters as much as optics: each new layer must register to the first over the whole wafer within a fraction of a micron, using the alignment flats/notches of Unit section 5. Below the resist, the wafer undergoes etching (wet acid etching is isotropic and undercuts; plasma/dry etching is anisotropic and preserves fine geometry) and deposition steps (CVD of polysilicon, SiO2, Si3N4; sputtered aluminium for interconnect).

(a) grow SiO₂ (b) resist, UV through mask (c) develop, etch window (d) dope / deposit SiO₂ UV dopant
Figure — one lithographic cycle: (a) grow the masking oxide; (b) coat photoresist and expose through a mask; (c) develop and etch a window in the oxide; (d) diffuse or deposit material through the window, then strip the resist.
Worked example · dies per wafer
A 200 mm wafer carries dies of 8 mm × 8 mm. Estimate the gross number of dies per wafer, the usable count after about 5% edge loss (partial dies at the circular rim cannot be used), and the number of good dies at an 80% process yield.
Die area: 8 × 8 = 64 mm².
Wafer area: πr² = π × 100² = 31,416 mm².
Gross count: 31,416/64 = 490.9 → ≈490 dies if the wafer were square.
Edge correction: partial dies around the circular rim are discarded: 490 × 0.95 ≈ 465 usable dies.
Good dies: 465 × 0.80 = 372 good dies per wafer.
Check: the edge penalty grows with die size relative to wafer diameter — a 20 mm die on the same wafer loses proportionally far more, which is one reason yields and economics push wafers ever larger.

8Diffusion and ion implantation

Doping the wafer is done two ways. Diffusion deposits dopant atoms at the surface (gas-phase, high-concentration "predeposition") and then drives them in at 1000–1200 °C, where they hop through lattice vacancies following Fick’s laws — the junction depth xj grows as the square root of drive-in time. Diffusion is cheap, batch-friendly and isotropic, spreading dopant under the mask edges (lateral diffusion) that limits fine geometry. Ion implantation accelerates ionised dopants (10–500 keV) and fires them into the wafer: the dose is counted by integrating the beam current, giving unheard-of dose accuracy, and the depth profile is set by accelerating voltage. Implantation scatters the crystal lattice, so an anneal (800–1000 °C) repairs the damage and activates the dopants; modern rapid thermal anneal does it in seconds to keep profiles shallow. Implantation is anisotropic, maskable and room-temperature — the default for fine-geometry doping — while diffusion survives in thick, deep, low-precision junctions.

Dose Q = ∫ ndop(x) dx [ions/cm²] = (I·t)/(q·A) for a beam of current I over time t on area A
Diffusion drive-in: xj ∝ √(D·t), D doubling roughly every 25–30 °C
Worked example · ion-implant dose and time
A 150 mm wafer is implanted with phosphorus at a dose of 5×1015 ions/cm². The accelerator delivers a singly charged (q = 1.6×10−19 C) beam of 1.0 mA. Find the total number of ions implanted and the implantation time.
Wafer area: A = πr² = π × (7.5 cm)² = 176.7 cm².
Total ions: N = Q·A = 5×1015 × 176.7 = 8.84×1017 ions.
Ion arrival rate: I/q = 1.0×10−3/1.6×10−19 = 6.25×1015 ions/s.
Time: t = N/(I/q) = 8.84×1017/6.25×1015 = 141.4 s ≈ 2 min 21 s.
Check: doubling the beam current halves the time; the current integration is exactly why implant doses are reproducible to a few percent across thousands of wafers — diffusion furnaces cannot match that control.

9Fabrication of the PN junction diode

The standard planar PN diode is built by the same cycle as in section 7, applied twice. Start with an n-type (ND ≈ 1016 cm−3) wafer: (1) grow a thick SiO2 masking layer; (2) lithographically open windows; (3) diffuse (or implant and drive) boron through the windows until the p-region depth reaches the wanted junction depth xj (≈1–5 µm) — everywhere else the oxide blocks the dopant; (4) grow a new oxide over the diffused region; (5) open contact windows to the p and n sides; (6) evaporate/sputter aluminium, pattern it photolithographically into the two contact pads, and alloy at 450–500 °C for ohmic contact; (7) passivate the surface with a final oxide or nitride. The junction "planarises" under the protecting oxide — the junction area is defined purely by the mask window geometry, which is the whole trick of planar technology.

The process sets the diode’s ratings: junction depth and surface doping fix the breakdown voltage (deeper, lighter-doped junctions break down at higher V), the mask window area fixes the current capacity (IF ≈ 1–2 A per mm² of junction), and the oxide passivation fixes the leakage. Screening away units outside the I–V specification window happens at wafer test (section 12).

Examiner’s checklist for "draw the fabrication steps of a PN diode": oxidation → window etching → p-diffusion → re-oxidation → contact windows → metallisation → alloy → passivate, with a labelled cross-section sketch after each step.

10Fabrication of the BJT

An npn planar BJT is the diode process iterated — three diffusions, or in modern plants implanted and annealed layers. Starting from an n+ substrate (low collector series resistance) on which a light n-type collector epitaxial layer has been grown: (1) grow oxide and open windows for the isolation grid; (2) diffuse p+ through them to surround each transistor island with reverse-biased pn isolation walls; (3) open the buried collector window and diffuse n+ beneath where the collector contact will sit; (4) the base diffusion: shallow p-type (boron) into the island, depth ≈1–2 µm; (5) the emitter diffusion: n+ (phosphorus or arsenic) inside the base window, leaving a narrow lightly doped base strip between emitter and collector — base width WB ≈ 0.5–1 µm, set by the difference of the two diffusion depths; (6) re-oxidise, open E, B and C contact windows, metallise and alloy. The final transistor is three stacked doped regions accessed from the top surface.

The doping profile is the design: emitter heavily doped (NE > NC > NB) for high injection efficiency, base light and thin for high β and speed, collector light in the epi layer for breakdown and low capacitance with an n+ path underneath for low resistance. Each additional mask level adds cost and yield risk — a discrete BJT needs 5–7 masks, a bipolar IC 10–15 because of the isolation wells.

Worked example · integrated resistor
A base-diffusion resistor is laid out over a region of sheet resistance Rs = 200 Ω/□ with length L = 100 µm and width W = 10 µm (contact resistance neglected). Find its value, and the new width needed to halve it while keeping the same length.
Number of squares: L/W = 100/10 = 10 squares.
Resistance: R = Rs × (L/W) = 200 × 10 = 2 kΩ.
To halve: R = 1 kΩ needs L/W = 1000/200 = 5 squares, so with L = 100 µm the width must be W = 100/5 = 20 µm.
Check: doubling the width halves the squares (10 → 5) at constant length — and quadruples the silicon area consumed, illustrating why large-value resistors are discouraged in monolithic design (they are replaced by transistor-based current sources).

11Fabrication of the MOSFET

The modern planar MOSFET (n-channel shown) starts from a p-type wafer. (1) Field isolation: thick oxide regions (LOCOS, or shallow-trench isolation in advanced nodes) separate transistors. (2) Gate: grow the thin gate oxide (historically 5–20 nm dry oxide; today deposited high-k dielectric) over the active area, deposit the polysilicon (or metal gate) on top, and pattern both by one mask — the gate stack becomes the alignment master. (3) Source/drain: lightly doped extensions are implanted, spacers are grown on the gate sides, then the heavy n+ source/drain implant is done using the gate and spacers as the mask. Because the implanted ions stop where the gate stops, the source/drain edges automatically sit flush against the gate edge — the self-aligned gate, the single most important idea in MOS processing, which eliminates the overlap capacitance an independent mask would create.

Gate length L defined by the gate mask, not by a diffusion depth — so L scaled from 10 µm (1970s) to nanometres; self-alignment removes gate–source/drain overlap capacitance

(4) Threshold adjust: a shallow implant through the gate oxide tunes VT. (5) Anneal to activate, deposit an insulating re-oxidation, open contact holes to S, D and gate, and metallise. CMOS processing simply repeats the MOSFET sequence in both polarities inside n-wells and p-wells, roughly doubling the mask count. The MOSFET is more lithography-dominated than the BJT: its performance is set by gate length and gate-oxide thickness — dimensions drawn by masks — rather than by diffusion depths, which is why MOS density scaling outpaced bipolar.

S (n+) D (n+) G (poly-Si) gate oxide (SiO₂) channel (inversion layer) p substrate gate length L
Figure — self-aligned n-channel MOSFET cross-section: the gate stack masks the n+ source/drain implants, so their edges meet the gate exactly; the inversion channel forms under the thin gate oxide when VGS > VT.

12Testing: wafer probing and yield

After all processing, the wafer goes to wafer sort: an automated prober steps a probe card across every die site and tests each chip electrically — continuity, parametric measurements on special test structures, then functional and speed tests at temperature. Failed dies are inked or mapped; the map drives binning (speed grades) and process control. Only good dies proceed to packaging, so wafer test is where yield economics are decided: the cost of a package is wasted on any die packaged blind.

Overall yield Y = Y1N for N process steps of individual yield Y1  |  die yield ≈ e−A·D (Seeds model) for die area A and defect density D

Two multiplicative factors govern the outcome. Process yield: if every one of N mask-and-process steps succeeds with probability Y1, the chance a wafer is fully correct is Y1N — compounding brutally with complexity. Die yield: larger dies collect more defects, so the probability of a clean die falls exponentially with area — the reason cost per function, not per chip, is the real metric of integration.

Worked example · composite process yield
A bipolar IC process has 8 masking levels, each achieved with 95% yield. Compare the overall process yield with an improved 98%-per-level process. What does each improvement of 1% per level buy at 8 levels, roughly?
Baseline: Y = 0.958. 0.952 = 0.9025, 0.954 = 0.90252 = 0.8145, 0.958 = 0.81452 = 0.6634 → 66.3%.
Improved: Y = 0.988 = e8·ln 0.98 = e−0.1616 = 0.851 → 85.1%.
Sensitivity: a 3% per-level improvement lifts the composite yield by 18.8 percentage points — because small per-level losses multiply. The lesson (and the exam point): fab economics obsess over every single step, since 1% per level saved compounds to roughly 8% more sellable wafers here, and far more at 20+ mask levels in modern CMOS.

13Bonding and packaging

Good dies are separated from the wafer by sawing or scribing along the street grid, then die-attached with conductive epoxy or eutectic solder into a leadframe or substrate cavity — the die pad doubles as the ground/thermal anchor. Electrical connection is made by wire bonding: gold or aluminium wires of 15–50 µm diameter, ultrasonically welded ball-to-pad (thermocompression/thermosonic bonding), from each chip pad to its leadframe finger. Advanced packages replace wires with flip-chip solder bumps across the whole die face (better power delivery, more I/O, but thermal-expansion matching required) and with tape-automated bonding.

The package then seals against moisture and contamination (moulded epoxy plastic for cost; hermetic ceramic or metal for reliability extremes) and dissipates device heat through the die pad — thermal resistance θJA is a headline package specification. Package families track the market: DIP for legacy through-hole, SOIC/QFP for surface mount, BGA for high pin counts, QFN for small footprints, and wafer-level packaging where interconnection is made before dicing. Finally every packaged unit is burned in and re-tested (screening infant mortalities), marked, and shipped — the last filter before the device meets the board.

Packaging is not an afterthought electrically: bond-wire inductance (nH per mm) limits high-speed and power designs, and the die–package thermal path sets the power rating. A brilliant chip in a careless package fails the datasheet.